<kbd id="yicbpmde"></kbd><address id="yicbpmde"><style id="yicbpmde"></style></address><button id="yicbpmde"></button>

              <kbd id="7xshjthn"></kbd><address id="7xshjthn"><style id="7xshjthn"></style></address><button id="7xshjthn"></button>

                      <kbd id="tl4nilqm"></kbd><address id="tl4nilqm"><style id="tl4nilqm"></style></address><button id="tl4nilqm"></button>

                              <kbd id="d5i2zu4r"></kbd><address id="d5i2zu4r"><style id="d5i2zu4r"></style></address><button id="d5i2zu4r"></button>

                                      <kbd id="odaprnec"></kbd><address id="odaprnec"><style id="odaprnec"></style></address><button id="odaprnec"></button>

                                              <kbd id="vksv1bz9"></kbd><address id="vksv1bz9"><style id="vksv1bz9"></style></address><button id="vksv1bz9"></button>

                                                      <kbd id="rzmlhe4n"></kbd><address id="rzmlhe4n"><style id="rzmlhe4n"></style></address><button id="rzmlhe4n"></button>

                                                          申博
                                                          您好,歡迎訪問中冶建研網站 !

                                                          CGM高鐵支座砂漿

                                                          CGM系列灌漿料


                                                               CGM灌漿料系列產品(以下簡稱CGM灌漿料)是以高強度材料爲骨料,以水泥作爲結合劑,輔以高流態、微膨脹、防離析等物質 ,經一定工藝加工而成的幹混砂漿。在現場使用時只需添加規定量的水攪拌均勻即可施工,簡便、快捷。
                                                              CGM灌漿料是中冶集團建築研究總院於1991年自主研發出的新型水泥基灌漿材料曾獲得多項國家、部委的科技進步獎和新產品證書。北京紐維遜建築工程技術有限公司是國內第一個灌漿料行業標準《水泥基灌漿材料施工技術規程》(YB/T9261-98)和國家標準《水泥基灌漿材料應用技術規範》(GB/T50448-2008)的編制單位 。目前,我公司CGM灌漿料產品已銷往全國各省、市、自治區  ,廣泛應用在冶金、石化、電力、煤炭、機械、建築、輕工、海工、路橋、環保、市政等領域的設備安裝、結構加固、建築維修的重大工程項目中 ,其優質的質量和良好的服務受到了客戶的好評 。
                                                            
                                                                                                    CGM灌漿料



                                                          資質、證書

                                                          CGM灌漿料


                                                          一產品特點:
                                                          1.塑性膨脹和硬化期膨脹的雙重效應 ,確保有效承載面(EBA) 大於90%,均勻傳遞荷載 。
                                                          2.大流動度、不泌水、不離析,施工更加簡便快捷  ,確保施工質量。
                                                          3.早強高強灌漿24小時後確保設備正常運行生產。
                                                          4.不含金屬膨脹源不腐蝕鋼筋 ,抗油滲、耐久性好 。

                                                          灌漿料


                                                          二、產品應用指南
                                                            1、設備基礎及鋼結構柱腳底板二次灌漿


                                                          灌漿層厚度 b(mm) 選用產品
                                                          5~20 CGM®380 系列產品
                                                          20~80 CGM®340 系列產品
                                                          50~200 CGM®300 系列產品
                                                          ≥ 150 CGM®270 系列產品
                                                           
                                                            2、地腳螺栓錨固灌漿柱杯口灌漿
                                                          灌漿層厚度 b(mm) 選用產品
                                                          15~80 CGM®340 、CGM®300 系列產品
                                                          ≥ 50 CGM®270 系列產品


                                                          3、混泥土結構加固灌漿:①加大截面法加固以及鋼結構柱(混泥土柱)杯口灌漿選用CGM270系列產品;②鋼板套法加固選用CGM380、CGM340系列產品(根據鋼板與柱壁間距)。
                                                                                               灌漿料

                                                          4、後張預應力混凝土結構孔道灌漿採用 CGM®-380(充分補償收縮 ,防止灌漿後孔道中形成“月牙效應”) 。
                                                          5、冬期施工灌漿
                                                                施工環境溫度爲 -15—5 ℃ 時,應採用CGM-340C、CGM-300D、CGM-270C 負溫早強型冬施專用灌漿料。
                                                           6、設備灌漿部位長期處於高溫環境,輻射溫度 500℃以下,可採用CGM-300E耐熱型灌漿料。

                                                          三、主要技術指標
                                                          CGM®-380 系列灌漿料

                                                              CGM®380A 預應力灌漿料 CGM®380B CGM®380C
                                                          流動度(mm) 初始值 ≥380  ≥380 ≥380
                                                          30min保留值 ≥ 340 ≥ 340 /
                                                          流錐法(S) 初始值 12 ~ 18s / /
                                                          30min保留值 12 ~ 18s
                                                          豎向膨脹率    (%) 3h 0.1~3.5 0.1~3.5 0.1~3.5
                                                          24h與3h膨脹值之差 0.02~0.5 0.02~0.5 0.02~0.5
                                                          抗壓強度
                                                          (MPa) 40×40×160mm 試體
                                                          2h / / 15
                                                          1d ≥ 20 ≥ 20 ≥ 25
                                                          3d ≥ 40 ≥ 40 ≥ 40
                                                          28d ≥ 60 ≥ 60 ≥ 60
                                                          泌水率 (%) 0 0 0
                                                          氯離子含量(%) ≤ 0.06 / /
                                                          對鋼筋有無鏽蝕作用
                                                          材料用量 (kg/m3) 1800 2000 2000
                                                          可施工時間 (min) 45 45 20
                                                          最低施工溫度(℃) 5 -5 5

                                                           CGM®-340 系列灌漿料
                                                          性能參數 CGM®
                                                          -340A
                                                          CGM®
                                                          -340B
                                                          CGM®-340C早強型 CGM®-340D負溫早強型 CGM®-340E耐熱型超 CGM®-340F高強型
                                                          流動度 (mm) 初始值 ≥345     ≥345 ≥345 ≥345 ≥345 ≥345
                                                          30min 保留值 ≥ 310 ≥ 310 / / ≥ 310 ≥ 310
                                                          豎向膨脹率 (%) 3h 0.1~3.5 0.1~3.5 0.1~3.5 0.1~3.5 0.1~3.5 0.1~3.5
                                                          24h 與 3h 膨脹值之差 0.02~0.5 0.02~0.5 0.02~0.5 0.02~0.5 0.02~0.5 0.02~0.5
                                                          抗壓強度
                                                          (MPa)40 × 40 × 160mm 試體( 標養 )
                                                          2h / / ≥ 15 / / /
                                                          1d ≥ 25 ≥ 30 ≥ 25 ≥ 25 ≥ 25 ≥ 25
                                                          3d ≥ 40 ≥ 45 ≥ 40 ≥ 40 ≥ 40 ≥ 40
                                                          28d ≥ 60 ≥ 80 ≥ 60 ≥ 60 ≥ 60 ≥ 60
                                                          抗壓強度 (MPa)
                                                          40 × 40 ×
                                                          160mm
                                                          試體(規定溫
                                                          度 -10℃)
                                                          -1d       ≥ 10    
                                                          -3d / / / ≥ 15 / /
                                                          -7+28d       ≥ 60    
                                                          抗壓強度(MPa) 40×40×160mm 試體(500℃ ×3h) 28d / / / / ≥ 70 /
                                                          熱震性(20 次) / / / / / 試件表面無脫落;浸水 / 後抗壓強度無顯著變化 /
                                                          泌水率(%) 0 0 0 0 0 0
                                                          材料用量 (kg/m3) 2200 2200 2200 2200 2200 2400
                                                          可施工時間 (min) 45 45 20 30 45 45
                                                          最低施工溫度(℃) -5 -5 5 15 -5 -5

                                                          CGM®-300 系列灌漿料
                                                            CGM-
                                                          300A
                                                          CGM-300B CGM-300C早強型 CGM-300D負溫早強型 CGM-300E耐熱型超 CGM-300F
                                                          高強型
                                                          流動度 (mm) 初始值 ≥300 ≥300 ≥300 ≥300 ≥300 ≥300
                                                          30min 保留值 ≥ 270 ≥ 270 / / ≥ 270 ≥ 270
                                                          豎向膨脹率 (%) 3h 0.1~3.5 0.1~3.5 0.1~3.5 0.1~3.5 0.1~3.5 0.1~3.5
                                                          24h 與
                                                          3h膨脹值之差
                                                          0.02~0.5 0.02~0.5 0.02~0.5 0.02~0.5 0.02~0.5 0.02~0.5
                                                          抗壓強度(MPa)
                                                           40 × 40 ×
                                                          160mm 試體
                                                          ( 標養 )
                                                          2h / / ≥ 15 / / /
                                                          1d ≥ 25 ≥ 30 ≥ 25 ≥ 25 ≥ 25 ≥ 35
                                                          3d ≥ 40 ≥ 45 ≥ 40 ≥ 40 ≥ 40 ≥ 50
                                                          28d ≥ 60 ≥ 80 ≥ 60 ≥ 60 ≥70 ≥ 90
                                                          抗壓強度(MPa) 40 × 40 × 160mm試體(規定溫度 -10℃) -1d       ≥ 10    
                                                          -3d / / / ≥ 15 / /
                                                          -7+28d       ≥ 60    
                                                          抗壓強度(MPa)
                                                          40 × 40 ×
                                                          160mm 試體
                                                          (500℃ ×3h)
                                                          28d / / / / ≥ 70 /
                                                          熱震性(20 次) / / / / / 試件表面無脫落 ;浸水後抗壓強度無
                                                          顯著變化
                                                          /
                                                          泌水率(%) 0 0 0 0 0 0
                                                          材料用量 (kg/m3) 2200 2200 2200 2200 2200 2400
                                                          可施工時間 (min) 45 45 20 30 45 45
                                                          最低施工溫度(℃) -5 -5 5 15 -5 -5

                                                          CGM®-270 系列灌漿料
                                                            CGM-
                                                          270A
                                                          CGM-
                                                          270B
                                                          CGM-270C早強型 CGM-270D負溫早強型 CGM-270E
                                                          耐熱型超
                                                          CGM-270F
                                                          高強型
                                                          坍落度 (mm) 初始值 ≥270 ≥270 ≥270 ≥270 ≥270 ≥270
                                                          30min 保留值 ≥ 240 ≥ 240 / / ≥ 240 ≥ 240
                                                          豎向膨脹率 (%) 3h 0.1~3.5 0.1~3.5 0.1~3.5 0.1~3.5 0.1~3.5 0.1~3.5
                                                          24h 與 3h 膨脹
                                                          值之差
                                                          0.02~0.5 0.02~0.5 0.02~0.5 0.02~0.5 0.02~0.5 0.02~0.5
                                                          抗壓強度 (MPa)
                                                           40 × 40 ×
                                                          160mm 試體 ( 標
                                                          養 )
                                                          2h / / ≥ 20 / / /
                                                          1d ≥ 25 ≥ 30 ≥ 25 ≥ 25 ≥ 25 ≥ 35
                                                          3d ≥ 40 ≥ 45 ≥ 40 ≥ 40 ≥ 40 ≥ 50
                                                          28d ≥ 60 ≥ 80 ≥ 60 ≥ 60 ≥70 ≥ 90
                                                          抗壓強度 (MPa)
                                                          40 × 40 ×
                                                          160mm 試體(規
                                                          定溫度 -10℃)
                                                          -1d / / / ≥ 10 / /
                                                          -3d / / / ≥ 15 / /
                                                          -7+28d / / / ≥ 60 / /
                                                          抗壓強度 (MPa)
                                                          40 × 40 ×
                                                          160mm 試體
                                                          (500℃ ×3h)
                                                          28d / / / / ≥ 70 /
                                                          熱震性(20 次) / / / / / 試件表面無脫落 ;浸水後抗壓強度無顯著變化 /
                                                          泌水率(%) 0 0 0 0 0 0
                                                          材料用量 (kg/m3) 2200 2200 2200 2200 2200 2400
                                                          可施工時間 (min) 45 45 20 30 45 45
                                                          最低施工溫度(℃) -5 -5 5 15 -5 -5

                                                          注:以上數據在標準實驗室條件下測得 。

                                                          四、施工方法
                                                          1、施工前應準備攪拌設備、養護物品和必要的工具 。
                                                          2、CGM灌漿料的拌合
                                                            (1)CGM灌漿料拌合時,加水量應按隨貨提供的產品合格證上的用水量加入,攪拌均勻即可使用。在滿足施工流動度的條件下儘量降低用水量 。嚴禁使用明顯沁水的攪和料進行灌漿。
                                                            (2)CGM灌漿料的拌合可採用機械攪拌或人工攪拌。推薦採用強制式機械攪拌方式 。
                                                            (3)每次攪拌量應視使用量多少而定,以保證 40 分鐘以內將拌合好的灌漿料用完 。
                                                            (4)冬期施工時 ,應採用不超過 60℃的熱水拌合灌漿料 ,漿體的入模溫度在 10℃以上。
                                                            (5)現場使用時 ,嚴禁在 CGM 灌漿料中摻入任何外加劑、外摻料。
                                                           3、地腳螺栓錨固
                                                            (1)地腳螺栓成孔時,基礎混凝土強度不得小於 20MPa,螺栓孔的水平偏差不得大於 5mm,垂直度偏差不得大於 5°,螺栓孔壁應粗糙。
                                                            (2)成孔後 ,應除去孔內雜物、申博孔的深度 ,並用水充分溼潤孔壁 。灌漿前應清除孔內積水 。
                                                            (3)將拌合好的CGM灌漿料灌入螺栓孔中,灌漿過程中嚴禁震搗 ,必要時可輕微插搗。灌漿結束後不得調整螺栓。
                                                            (4)灌漿施工不易直接灌入時,宜採用流槽輔助施工。
                                                           4、設備基礎二次灌漿
                                                            (1)設備基礎表面應進行鑿毛處理 。清掃設備基礎表面  ,不得有碎石、浮漿、浮灰、油污和脫模劑等雜物 。灌漿前 24 小時,設備基礎表面應充分溼潤 。灌漿前 1 小時 ,清除積水  。
                                                            (2)按灌漿施工圖支設模板。模板與基礎、模板與模板間的接縫處用水泥漿、膠帶等封縫 ,達到整體模板不漏水的程度。模板與設備底座四周的水平距離應控制在 100mm 左右 。模板頂部標高應高出設備底座上表面 50mm。
                                                            (3)較長設備或軌道基礎的灌漿應採用分段施工 。即採用跳倉法施工,每段長度不應超過 5m ,大型設備灌漿必須採用壓力灌漿設備 ,確保連續灌漿 。
                                                            (4)應從一側或相鄰的兩側多點進行灌漿,直至從另一側溢出爲止,以利於灌漿過程中的排氣。不得從四側同時進行灌漿。
                                                            (5)灌漿開始後,必須連續進行 ,不能間斷  。並儘可能縮短灌漿時間 。
                                                            (6)在灌漿過程中嚴禁振搗。必要時可用灌漿助推器沿灌漿層底部推動 CGM灌漿料  ,嚴禁從灌漿層的中、上部推動 ,以確保灌漿層的勻質性  。
                                                            (7)設備基礎灌漿完畢後 ,應在灌漿後 3~6 小時沿設備邊緣向外切45℃斜角(見下圖)以防止自由端產生裂縫。如無法進行切邊處理,應在灌漿後 3~6 小時用抹刀將灌漿層表面壓光。(該部位產生的細小裂縫對設備運轉穩定性未報告有不良影響)。
                                                                                             灌漿料

                                                          5、混凝土結構加固
                                                          (1) 將拌合好的 CGM灌漿料灌入已支設好的模板中 ;
                                                          (2) 灌漿過程中 ,根據需要可適當敲擊模板或振搗 ;
                                                          (3) 拆模時間應符合本施工方法下表的規定 。

                                                          日最低氣溫(℃ ) 拆模時間(h) 養護時間(d)
                                                          - 10~0 96 14
                                                          0~5 72 10
                                                          5~15 48 7
                                                          ≥ 15 24 7



                                                          五、施工養護
                                                           1、自然養護
                                                           (1)灌漿完畢後裸露部分應及時噴灑水養護或覆蓋塑料薄膜 ,並加蓋溼草袋保持溼潤。
                                                           (2)澆水養護時間不得少於 7 天,澆水次數應保持灌漿材料處於溼潤狀態。當採用快凝快硬型 CGM灌漿料時 ,養護應根據產品要求的方法執行 。
                                                           2、冬期養護
                                                          (1)冬期施工時灌漿工程對強度增長無特殊要求時,灌漿完畢後裸露部分應及時覆蓋塑料薄膜並加蓋保溫材料。起始養護溫度不應低於 5℃。在負溫條件養護時不得澆水;
                                                          (2)拆模後灌漿料表面溫度與環境溫度之差大於 20℃時 ,應採用保溫材料覆蓋養護 ;
                                                          (3)如環境溫度低於產品要求的最低施工溫度或需要加快強度增長時,可採用人工加熱養護方式;養護措施應符合現行《建築工程冬期施工規程》(JGJ104)的有關規定 。
                                                           3、CGM灌漿料達到拆模時間後 ,可進行設備安裝 ,具體時間見下表。


                                                          日最低氣溫(℃ ) 拆模時間(h) 養護時間(d)
                                                          - 10~0 96 14
                                                          0~5 72 10
                                                          5~15 48 7
                                                          ≥ 15 24 7

                                                          4、在設備基礎灌漿完畢後 ,如有要剔除部分,可在灌漿完畢 3—6小時後,即灌漿層硬化前用抹刀或鐵鍬等工具輕輕剷除 。
                                                          5、不得將正在運轉的機器的震動傳給設備基礎 ,在二次灌漿後應停機24—36小時,以避免損壞未結硬的灌漿層。